Silicon Rose After the Repair.
Aluminium Didn’t.

Silicon rose from 5 to 29 ppm after the gearbox cover was resealed. Does the oil report justify draining 60 litres?

Illustration of a bolted gearbox cover with a narrow grey bead of silicone squeezed out along the machined joint.
Illustration of silicone squeezed from the bolted cover joint. In this worked example, the oil sample comes a week later.
In this article

The top cover went back on with a bead of grey silicone, and some of it squeezed out along the joint. In this worked example, the first oil sample, taken warm from the usual valve a week after restart, showed silicon at 29 ppm against 5 ppm before the job. The lab comment says “possible dirt ingress”.

That comment can start an oil change, a flush and a search for the way in. Nobody had told the lab about the sealant.

The gearbox is a splash-lubricated industrial helical unit holding 60 litres of ISO VG 220 mineral gear oil. The repair was to the cover joint, which had been weeping oil until the level was about 6 litres low. The cover came off without draining. While the housing was open, the gear mesh was inspected and the breather was off. After restart, and before that sample, 6 litres of the same oil brought the level back up.

On the same report, aluminium held at 2 ppm, iron was steady and the ISO 4406 code stayed at 18/16/13. Silicon has more than one source, and three of them were present during this job. The short answer: leave the oil in for now and run the checks below.

Three sources, one element

ALS’s guide to oil analysis results lists silicon twice: as an antifoam additive, and as a contaminant from dirt or gasket and sealant material. That gives three candidates. Dirt could have entered while the housing was open, or could still be entering past a disturbed breather. Silicone could have come off the fresh sealant. Or the top-up could have carried antifoam in with it.

The top-up is the quickest to test, because it is arithmetic. On its own, it mixes 6 litres of new oil into 54 litres at 5 ppm. Take 4 ppm for the new oil, a worked value until you measure the drum. The mix is (54 × 5 + 6 × 4) ÷ 60 = 4.9 ppm. Even with 40 ppm in the new oil, the mix only reaches 8.5 ppm. To make 29 on its own, the new oil would need about 245 ppm.

Ask what rose with the silicon

Look for a partner before you call it dirt. ALS lists aluminium as a sign of dirt when it appears “in combination with silicon”. Here silicon rose by 24 ppm and aluminium did not move.

How much aluminium comes with the silicon depends on the dust, so compare with a dirt event confirmed on your own site, not with a ratio borrowed from another plant. In this example the plant has one confirmed dirt event, on a sister gearbox with a cracked breather. Silicon rose 14 ppm, aluminium rose 6 ppm and the 4 µm particle code went up two steps.

Particles are the third check. Each step up in an ISO 4406 code number doubles the count, so those two steps meant about four times as many particles. This gearbox’s code did not move.

When dirt got into the sister gearbox, it brought aluminium and particles with it. This time the silicon came alone.

Two gearboxes before and after, plotted on a common ppm scale. Silicon in the resealed gearbox rose from 5 to 29 ppm while aluminium stayed at 2 ppm and ISO cleanliness stayed 18/16/13. In the known dirt event, silicon rose from 6 to 20 ppm, aluminium from 2 to 8 ppm, and the ISO code from 17/15/12 to 19/17/13. The shaded band marks the 4.9 to 8.5 ppm predicted by the repair top-up alone.
The hatched band is what the 6-litre top-up alone would give with 4 to 40 ppm silicon in the new oil; reaching 29 ppm would take about 245 ppm. All values are from the worked example.

So far the sealant fits better than dirt. It is not proven yet, because an unchanged 2 ppm cannot rule out grit.

What the report cannot see

If your lab runs ICP to ASTM D5185, the method’s scope says it is calibrated with oil-soluble metals and gives low results for particles larger than a few micrometres. Our 12 November article covers that limit for iron. It applies here too: ICP alone could miss coarse grit, which is why the unchanged particle count matters, and why it is worth seeing what the particles actually are.

So ask for a filter patch. ALS describes collecting debris on a 0.8 to 5.0 µm membrane and examining it under a microscope. ExxonMobil’s used-oil guide, written for jet engines, says inspecting the oil filter will often show whether the silicon is silicate (dirt) or silicone. This gearbox has no filter to cut open, so the patch is the closest check available. Ask the lab whether the debris includes mineral grit or sealant. Send a sample from the drum the top-up came from as well, so the worked 4 ppm becomes a measured figure.

Explanation Aluminium 4 µm particle code Filter patch Next sample
Silicone from the sealant Stays level May not move No mineral grit; sealant flakes possible Silicon levels off; aluminium and particles stay flat
Dirt let in during the job Rises with silicon Rises Mineral grit Silicon stops rising
Dirt still entering at the breather Rises with silicon Rises Mineral grit Silicon, aluminium and particles keep rising
This gearbox so far 2 ppm, unchanged 18, unchanged Not yet done Not yet taken
  • Explanation
    Silicone from the sealant
    Aluminium
    Stays level
    4 µm particle code
    May not move
    Filter patch
    No mineral grit; sealant flakes possible
    Next sample
    Silicon levels off; aluminium and particles stay flat
  • Explanation
    Dirt let in during the job
    Aluminium
    Rises with silicon
    4 µm particle code
    Rises
    Filter patch
    Mineral grit
    Next sample
    Silicon stops rising
  • Explanation
    Dirt still entering at the breather
    Aluminium
    Rises with silicon
    4 µm particle code
    Rises
    Filter patch
    Mineral grit
    Next sample
    Silicon, aluminium and particles keep rising
  • Explanation
    This gearbox so far
    Aluminium
    2 ppm, unchanged
    4 µm particle code
    18, unchanged
    Filter patch
    Not yet done
    Next sample
    Not yet taken

Hold the drain, check the breather

Both mistakes cost something. Read dirt as sealant and grit keeps passing through the gear mesh and bearings while an open breather path lets more in. Read sealant as dirt and the plant drains 60 litres of VG 220, flushes the housing and reworks a breather that was never the problem. The next silicon comment then gets a little less attention, and that one may be real.

Sealant is not harmless either. The same ExxonMobil guide warns that high levels of sealant silicone can cause foaming, and says a foam test on the used oil may be needed when silicone is suspected. Our 5 November article describes the test.

A one-time source stops adding silicon. An open path keeps adding silicon, aluminium and particles together.

Before you drain: the checks, in order

  1. Today, at your desk. Redo the top-up sum. Tell the lab about the sealant, the open cover and the top-up, and ask what change in silicon it treats as real.
  2. Today, at the gearbox. Isolate the drive, then check the breather: the right part, seated and sealed, not cracked, with nothing left open where it came off. With the guards back on and the gearbox running, look for foam at the sight glass.
  3. This week, from the lab. A filter patch, a foam test, and silicon in the top-up drum.
  4. Next sample, sooner than normal, same valve. Compare silicon, aluminium, iron and the 4 µm code with this report.

If the patch shows no mineral grit and silicon is no higher next time, record a sealant event against the trend and leave the oil in. If it shows grit, or silicon, aluminium and the 4 µm code climb together, treat it as dirt: close the path, then clean or change the oil. If only silicon is higher again, neither rule is met. Do not drain on silicon alone: recheck the breather and resample once more. A fresh bead may still be giving up silicone, a possibility to test, not a sourced rate.

The lab wrote “possible dirt ingress” from the numbers alone. It never saw the bead. Put the job, the sealant and the top-up on the next sample form.

References

Explore more Insights

New field notes

Get one practical lubrication field note each month.

Clear guidance on lubrication, oil analysis and reliability improvement. No daily emails.

Trusted across critical operations.

Camso logo
Bajaj logo
Oman Methanol logo
General Mills logo
Normet logo
Geo-Chem logo
WearCheck logo
Predict Technologies logo
Rohit Enterprises logo
Emami logo
Hero logo
ENOC logo
Total logo
Tata Steel logo
Dow Chemical logo
Orient Cement logo
Kuwait Oil Company logo
Petronet logo
SAS logo
Vedanta logo
Pfizer logo
Vestas logo
Maruti Suzuki logo
MJL Bangladesh logo
Emirates Global Aluminium logo
Siam Cement Group logo
GASCO logo
Reliance logo
Chevron logo
BPCL logo
Essar Steel logo
NTPC logo